Jewelry Plaster
bg-title1-h1

Technical Help

Trouble Shooting

Investment Powder

Problem

Cause

Solutions

Bubbles

Trouble-Bubbles

In correct water / powder ratio (Investment too thick. Too little water)

Recommended water to powder ratio Vacuum mixing 38:100 / Conventional mixing 40:100

Work time of investment not too less

Appropriate time: 2-3 mins

Work time of investment not too long

Work cycle too long. Investment is starting to thicken while still being vacuumed Bubbles

Vacuum machine faulty-Vacuum leaks

Flashing or Finning

Trouble-Flashing-Finning

Incorrect water/ powder ratio (Too much water)

Recommended water to powder ratio Vacuum mixing 38:100 / Conventional mixing 40:100

Failure of conveyor belts
( Centrifugal casting) Over pressure (Vacuum casting)

Spin speed is too fast. Torque setting have to match spin speed.

Mixing time not long enough

Appropriate time : 3-4 mins

Overheat metal melting

Rough surfaces

Trouble-Rough-Surfaces

Stream de-wax for too less

Appropriate time 60 mins

Stream de-wax for too long

Appropriate time 60 mins

Flasks put in furnace too soon after mixing

Appropriate time 45-60 mins

Furnaces temperature is too high

Dewax too low temperature/ Lost wax time not long enough *Burnout Oven

Burnout temperature : 220°C250°C
Appropriate time :
60 mins

Sand Casting

Trouble-Sand-Casting

Less mixing time

Appropriate time 2-3 mins

Over casting temperature

Furnaces Temperature is too high

Lost wax process not long enough

Appropriate 60 mins

Cleanliness of wax piece

White bensin

Finning

Trouble-Finning

Furnace temperature is too high

Incorrect water/ powder ratio(Too much water)

Recommended water to powder ratio Vacuum mixing 38:100 / Conventional mixing 40:100

Furnaces failure

Moving flask too soon after mixing

Appropriate time 45 mins

Investment cracking

Room temperature is too low/ Too much humidity

Incomplete casting

Trouble-Incomplete-Casting

Defective patturn-Wax tree too hight

The maimum tree height should be between 0.5 inch shorter than the fill level of the flask.

Flaws in a plaster mould

Failure of conveyor belts ( Centrifugal casting)

Over pressuer ( Vacuum casting)

A mixture of plaster and group up old moulds

Incorrect water/ powder ratio ( Too much water)

Recommended water to powder ratio Vacuum mixing 38:100 / Conventional mixing 40: 100

Gas porosity

Trouble-Gas-Porosity

Incomplete burnout * a minimum of ten hours

Furnaces failure

Calibrate it once every 3-4 months







meun-download
menu facebook
menu twitter

Copyright © 2013 Jewelry Plaster. All Rights Reserved.

322/5-6 1st Floor, Bangkok Gem & jelelry Tower Surawong Road, Bangrak Bangkok 10500 Thailand
Tel: 02-2671178, Fax: 02-2671178, Email: jpl@jewelryplaster.com